Table 5: Flexural and compressive strength test.

Recycled mortar Dosage
1:3 1:4
RA Type Test(MPa) 50% 75% 100% 50% 75% 100%
RA 1 Flexural 5.13 4.77 4.02 3.47 3.24 3.02
Compressive 17.62 15.44 14.70 12.51 10.11 9.23
RA 2 Flexural 5.44 5.12 4.78 3.78 3.21 3.27
Compressive 20.34 17.86 15.23 12.67 11.91 10.42
NA Flexural - - 5.74 - - 4.12
Compressive - - 23.11 - - 17.52