Table 8: Effect of flexural steel reinforcement ratio on the ultimate failure load.

Slab
Designation
ρ Pcr
(kN)
Pu
(kN)
Pcr/ Pu ΔPcr % ΔPu %
NCS1-0-50 0.0033 9 29 0.31 33 45
NCS2-0-50 0.0066 12 42 0.28
NCS1-0-70 0.0033 12 41 0.29 25 37
NCS2-0-70 0.0066 15 56 0.28
MRPCS1-0-50 0.0033 21 73 0.29 43 33
MRPCS2-0-50 0.0066 30 97 0.31
MRPCS1-0-70 0.0033 35 128 0.27 12 14
MRPCS2-0-70 0.0066 39 146 0.27
MRPCS1-0.4-50 0.0033 26 106 0.25 27 7
MRPCS2-0.4-50 0.0066 33 112 0.29
MRPCS1-0.4-70 0.0033 43 189 0.23 0 -20
MRPCS2-0.4-70 0.0066 43 152 0.28
MRPCS1-0.8-50 0.0033 32 119 0.27 12.5 3
MRPCS2-0.8-50 0.0066 36 122 0.29
MRPCS1-0.8-70 0.0033 43 158 0.27 35 53
MRPCS2-0.8-70 0.0066 58 242 0.24