Table 2: Mean values (±SD) of coping fit (in µm) at the experimental measurement locations.

Measurement Location CAD-CAM Zirconia CAD-CAM Lithium Disilicate Heat Pressed Lithium Disilicate
Mean Value (±SD) Mean Value (±SD) Mean Value (±SD)
MG1 63 (±32) 65 (±17) 89 (±42)
FL1 71 (±16) 69 (±20) 86 (±18)
AW1 75 (±21) 71 (±18) 97 (±26)
BC 111 (±21) 124 (±32) 99 (±16)
OCF 116 (±32) 123 (±25) 91 (±39)
LC 125 (±25) 129 (±31) 108 (±32)
AW2 76 (±25) 74 (±24) 88 (±14)
FL2 79 (±14) 71 (±24) 84 (±26)
MG2 69 (±33) 68 (±36) 82 (±22)